CN103572064A - 一种稀土铅渣中富集铅及回收稀土的方法 - Google Patents
一种稀土铅渣中富集铅及回收稀土的方法 Download PDFInfo
- Publication number
- CN103572064A CN103572064A CN201310580259.3A CN201310580259A CN103572064A CN 103572064 A CN103572064 A CN 103572064A CN 201310580259 A CN201310580259 A CN 201310580259A CN 103572064 A CN103572064 A CN 103572064A
- Authority
- CN
- China
- Prior art keywords
- rare earth
- lead
- enriched
- recovering
- lead skim
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
本发明公开了一种稀土铅渣中富集铅及回收稀土的方法,包括如下步骤:(1)将硫化钠沉淀稀土得到的稀土铅渣在750-850℃进行焙烧;(2)向焙烧后的稀土铅渣中加入1-1.5mol/L的硫酸,80-90℃浸取40分钟以上;(3)将步骤(2)处理后的产物进行固液分离,上清液经碱转、酸溶后提取稀土;固体经水洗后得到铅富集物。本发明的方法大大减小了含铅废物的处理难度和成本,可将铅渣中所含的40%稀土提取出来。
Description
技术领域
本发明属于稀土领域,具体涉及一种稀土铅渣中富集铅及回收稀土的方法。
背景技术
现有稀土提纯方法法中,用硫化钠除去稀土中的铅,铅渣生成过程中带有40%稀土化合物和大量的Fe、Du、Ba、Ga等金属离子;后续铅渣处理成本高,稀土资源大量浪费,环境污染严重。
发明内容
本发明目的是提供一种稀土铅渣中富集铅及回收稀土的方法,解决现有的工艺存在的处理成本高、稀土资源大量浪费,环境污染严重的问题。
本发明的技术方案为:
一种稀土铅渣中富集铅及回收稀土的方法,包括如下步骤:
(1)将硫化钠沉淀稀土得到的稀土铅渣在750-850℃进行焙烧;
(2)向焙烧后的稀土铅渣中加入1-1.5mol/L的硫酸,80-90℃浸取40分钟以上;
(3)将步骤(2)处理后的产物进行固液分离,上清液经碱转、酸溶后提取稀土;固体经水洗后得到铅富集物。
进一步地,所述碱转的方法为:2-2.5mol/L NaOH加热反应7-9小时。
进一步地,所述酸溶的方法为:1-1.5mol/L的盐酸浸取40分钟以上。
进一步地,步骤(1)中的焙烧温度为800℃。
进一步地,步骤(2)中加入硫酸的浓度为1mol/L,浸取时间1小时以上。
本发明与现有技术相比具有如下优点:
本发明的方法大大减小了含铅废物的处理难度和成本,可将铅渣中所含的40%稀土提取出来,根据年生产10000t稀土能力计算,回收利用稀土40t,经济收益4000000元 。铅渣经处理后铅渣量每年减少 40t,减少铅渣处理费用180000元。
具体实施方式
实施例1
一种稀土铅渣中富集铅及回收稀土的方法,包括如下步骤:
(1)将硫化钠沉淀稀土得到的稀土铅渣在750℃进行焙烧;
(2)向焙烧后的稀土铅渣中加入1.5mol/L的硫酸, 90℃浸取40分钟;
(3)将步骤(2)处理后的上清液虹吸到另外的反应罐中,经碱转,酸溶,除杂等提取稀土;碱转的方法为:2mol/L NaOH加热反应9小时,酸溶的方法为: 1.5mol/L的盐酸浸取40分钟。固体经水洗后得到铅富集物。
实施例2
一种稀土铅渣中富集铅及回收稀土的方法,包括如下步骤:
(1)将硫化钠沉淀稀土得到的稀土铅渣在850℃进行焙烧;
(2)向焙烧后的稀土铅渣中加入1mol/L的硫酸, 80℃浸取50分钟;
(3)将步骤(2)处理后的上清液虹吸到另外的反应罐中,经碱转,酸溶,除杂等提取稀土;碱转的方法为:2.5mol/L NaOH加热反应7小时,酸溶的方法为: 1mol/L的盐酸浸取50分钟。固体经水洗后得到铅富集物。
实施例3
一种稀土铅渣中富集铅及回收稀土的方法,包括如下步骤:
(1)将硫化钠沉淀稀土得到的稀土铅渣在800℃进行焙烧;
(2)向焙烧后的稀土铅渣中加入1.25mol/L的硫酸, 85℃浸取50分钟;
(3)将步骤(2)处理后的上清液虹吸到另外的反应罐中,经碱转,酸溶,除杂等提取稀土;碱转的方法为:2.3mol/L NaOH加热反应7小时,酸溶的方法为: 1.2mol/L的盐酸浸取45分钟。固体经水洗后得到铅富集物。
Claims (5)
1. 一种稀土铅渣中富集铅及回收稀土的方法,其特征在于,包括如下步骤:
(1)将硫化钠沉淀稀土得到的稀土铅渣在750-850℃进行焙烧;
(2)向焙烧后的稀土铅渣中加入1-1.5mol/L的硫酸,80-90℃浸取40分钟以上;
(3)将步骤(2)处理后的产物进行固液分离,上清液经碱转、酸溶后提取稀土;固体经水洗后得到铅富集物。
2. 根据权利要求1所述的一种稀土铅渣中富集铅及回收稀土的方法,其特征在于,所述碱转的方法为:2-2.5mol/L NaOH加热反应7-9小时。
3.根据权利要求1所述的一种稀土铅渣中富集铅及回收稀土的方法,其特征在于,所述酸溶的方法为:1-1.5mol/L的盐酸浸取40分钟以上。
4.根据权利要求1所述的一种稀土铅渣中富集铅及回收稀土的方法,其特征在于,步骤(1)中的焙烧温度为800℃。
5.根据权利要求1所述的一种稀土铅渣中富集铅及回收稀土的方法,其特征在于,步骤(2)中加入硫酸的浓度为1mol/L,浸取时间1小时以上。